Wrought aluminum alloys (1xxx)

Dr. Dmitri Kopeliovich

According to the Wrought aluminum alloys designation system, alloys of this series are designated 1xxx.

This group includes aluminum of various grades of purity: 99.0% to 99.99% of aluminum.

The following elements may be present in the alloys as impurities: silicon (Si) and iron (Fe) as major impurities and also copper (Cu), manganese (Mn), magnesium (Mg), zinc (Zn), titanium (Ti) and others.

Alloys of this series have low mechanical strength, high ductility, excellent corrosion resistance and high electrical conductivity.

The alloys may be strengthened by cold work (strain hardening).

Aluminum from this group is used for manufacturing electric wires, chemical equipment, foil and decorative products.

Chemical compositions of some wrought aluminum alloys of 1xxx series

Designation Si,% Fe,% Cu,% Mn,% Mg,% Zn,% Ti,% Others,% Al, % min
1050 0.25 0.4 0.05 0.05 0.05 0.05 0.03 0.03 99.50
1060 0.25 0.35 0.05 0.03 0.03 0.05 0.03 0.03 99.60
1100 0.95 Si + Fe 0.05-0.2 0.05 - 0.1 - 0.15 99.00
1145 0.55 Si + Fe 0.05 0.05 0.05 0.05 0.03 0.03 99.45
1200 1.00 Si + Fe 0.05 0.05 - 0.1 0.05 0.15 99.00
1230 0.70 Si + Fe 0.1 0.05 0.05 0.1 0.03 0.03 99.30
1350 0.10 0.40 0.05 0.01 - 0.05 - 0.11 99.50

Properties of some wrought aluminum alloys of 1xxx series