Main page
About us
Sliding Bearings Consulting
Advertising Opportunities
to Wrought aluminum alloys (1xxx)
to Properties of aluminum alloys
(submitted by the website administration)
Wrought aluminum alloy 1060 | ||||
Chemical composition: Si=0.25%, Fe=0.35%, Al = 99.6% min | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 2.705 *10³ | kg/m³ | 169 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 69 | GPa | 10000 | ksi |
Thermal expansion (20 ºC) | 23.6*10-6 | ºCˉ¹ | 13.1*10-6 | in/(in* ºF) |
Specific heat capacity | 900 | J/(kg*K) | 0.215 | BTU/(lb*ºF) |
Thermal conductivity | 231 | W/(m*K) | 1600 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 2.81*10-8 | Ohm*m | 2.81*10-6 | Ohm*cm |
Tensile strength (annealed) | 69 | MPa | 10000 | psi |
Yield strength (annealed) | 28 | MPa | 4000 | psi |
Elongation (annealed) | 43 | % | 43 | % |
Shear strength (annealed) | 48 | MPa | 7000 | psi |
Fatigue strength (annealed) | 21 | MPa | 3000 | psi |
Hardness (annealed) | 19 | HB | 19 | HB |
Tensile strength (H16) | 110 | MPa | 16000 | psi |
Yield strength (H16) | 103 | MPa | 15000 | psi |
Elongation (H16) | 8 | % | 8 | % |
Shear strength (H16) | 69 | MPa | 10000 | psi |
Fatigue strength (H16) | 45 | MPa | 6500 | psi |
Hardness (H16) | 30 | HB | 30 | HB |
Annealing temperature | 343 | ºC | 650 | ºF |