USA: AISI T15, UK: BT15, Sweden: USA T15, Germany: 1.3202, Japan: SKH10 | ||||
Chemical composition: C=1.6%, Mn=0.3%, W=12%, Si=0.3%, Cr=4%, V=5%, Co=5% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.19 *10³ | kg/m³ | 511.2 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 214 | GPa | 31000 | ksi |
Thermal expansion (20 ºC) | 9.9*10-6 | ºCˉ¹ | 5.5*10-6 | in/(in* ºF) |
Specific heat capacity | 461 | J/(kg*K) | 0.11 | BTU/(lb*ºF) |
Thermal conductivity | 20.9 | W/(m*K) | 147 | BTU*in/(hr*ft²*ºF) |
Annealing temperature | 870...890 | ºC | 1600...1630 | ºF |
Quenching temperature | 1165-1235 | ºC | 2125-2250 | ºF |
Tempering temperature | 540...650 | ºC | 1000...1200 | ºF |
Hardness (annealed) | 56 | RC | 56 | RC |
Hardness (hardened) | 68 | RC | 68 | RC |
Quenching medium | Oil, air or salt | |||
Hardening depth | High | |||
Resistivity to distortion | Medium | |||
Resistivity to cracking | Medium | |||
Machinability | Medium (may be improved by addition of sulfur up to 0.22%) | |||
Toughness | Low | |||
Wear resistance | Very high |