SubsTech     
SubsTech     
Command disabled: index

to Non-heat-treatable nickel-chromium-iron alloys
to Properties of nickel alloys

Non-heat-treatable nickel-chromium-iron alloy Inconel 600

(submitted by the website administration)

Non-heat-treatable Nickel-Chromium-Iron Alloy Inconel 600
Chemical composition: Cr=15.5%, Fe=2.5%, Ni=72% min.
Property Value in metric unit Value in US unit
Density 8.47 *10³ kg/m³ 529 lb/ft³
Modulus of elasticity 207 GPa 30000 ksi
Thermal expansion (20 ºC) 13.3*10-6 ºCˉ¹ 7.4*10-6 in/(in* ºF)
Specific heat capacity 444 J/(kg*K) 0.106 BTU/(lb*ºF)
Thermal conductivity 14.9 W/(m*K) 103 BTU*in/(hr*ft²*ºF)
Electric resistivity 103*10-8 Ohm*m 103*10-6 Ohm*cm
Tensile strength (annealed) 655 MPa 95000 psi
Yield strength (annealed) 310 MPa 45000 psi
Elongation (annealed) 45 % 45 %
Liquidus temperature 1354 ºC 2470 ºF
Solidus temperature 1350 ºC 2460 ºF