Thermoplastic | ||||
Polysulfone (PSF) | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 1.25 *10³ | kg/m³ | 78.0 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 2.61 | GPa | 375 | ksi |
Tensile strength | 68 | MPa | 9800 | psi |
Elongation | 75 | % | 75 | % |
Flexural strength | 115 | MPa | 16500 | psi |
Thermal expansion (20 ºC) | 56*10-6 | ºCˉ¹ | 31*10-6 | in/(in* ºF) |
Thermal conductivity | 0.26 | W/(m*K) | 1.80 | BTU*in/(hr*ft²*ºF) |
Glass transition temperature | 190 | ºC | 375 | ºF |
Maximum work temperature | 160 | ºC | 320 | ºF |
Electric resistivity | 1.015*10-3 | Ohm*m | 1.015*10-1 | Ohm*cm |
Dielectric constant | 3.1 | - | 3.1 | - |
Applications: microwave cookware, medical equipment, chemical pumps, automotive components.