Wrought copper alloy C77000 (Nickel Silver 55-18)
Chemical composition: Ni=18%, Zn=27%, Cu=55%
Property Value in metric unit Value in US unit
Density 8.69*10³ kg/m³ 542 lb/ft³
Modulus of elasticity 124 GPa 18000 ksi
Thermal expansion (20 ºC) 16.7*10-6 ºCˉ¹ 9.3*10-6 in/(in* ºF)
Specific heat capacity 377 J/(kg*K) 0.090 BTU/(lb*ºF)
Thermal conductivity 29.4 W/(m*K) 204 BTU*in/(hr*ft²*ºF)
Electric resistivity 31.4*10-8 Ohm*m 31.4*10-6 Ohm*cm
Tensile strength (annealed) 414 MPa 60000 psi
Yield strength (annealed) 186 MPa 27000 psi
Elongation (annealed) 40 % 40 %
Hardness (annealed) 55 RB 55 RB
Tensile strength (cold work) 745 MPa 108000 psi
Yield strength (cold work) 621 MPa 90000 psi
Elongation (cold work) 2 % 2 %
Hardness (cold work) 96 RB 96 RB
Annealing temperature 600-850 ºC 1100-1500 ºF
Liquidus temperature 1054 ºC 1930 ºF