Cast copper C80100 (Copper)
Chemical composition: Cu = 99.95% min
Property Value in metric unit Value in US unit
Density 8.94 *10³ kg/m³ 558 lb/ft³
Modulus of elasticity 117 GPa 17000 ksi
Thermal expansion (20 ºC) 16.9*10-6 ºCˉ¹ 9.4*10-6 in/(in* ºF)
Specific heat capacity 394 J/(kg*K) 0.092 BTU/(lb*ºF)
Thermal conductivity 391 W/(m*K) 2712 BTU*in/(hr*ft²*ºF)
Electric resistivity 1.72*10-8 Ohm*m 1.72*10-6 Ohm*cm
Tensile strength ( mold cast) 172 MPa 25000 psi
Yield strength (mold cast) 62 MPa 9000 psi
Elongation (mold cast) 40 % 40 %
Fatigue strength (mold cast) 62 MPa 9000 psi
Hardness (mold cast) 44 HB(500) 44 HB(500)
Liquidus temperature 1083 ºC 1981 ºF
Solidus temperature 1064 ºC 1948 ºF