Cast copper alloy C81500 (Chromium Copper) | ||||
Chemical composition: Cr=1.0%, Cu = 99.0% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.82 *10³ | kg/m³ | 551 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 111 | GPa | 16000 | ksi |
Thermal expansion (20 ºC) | 17.1*10-6 | ºCˉ¹ | 9.5*10-6 | in/(in* ºF) |
Specific heat capacity | 377 | J/(kg*K) | 0.09 | BTU/(lb*ºF) |
Thermal conductivity | 315 | W/(m*K) | 2184 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 2.87*10-8 | Ohm*m | 2.87*10-6 | Ohm*cm |
Tensile strength (sand cast, solution treated and aged) | 351 | MPa | 50000 | psi |
Yield strength (sand cast, solution treated and aged) | 276 | MPa | 40000 | psi |
Elongation (sand cast, solution treated and aged) | 17 | % | 17 | % |
Fatigue strength (sand cast, solution treated and aged) | 103 | MPa | 15000 | psi |
Hardness (sand cast, solution treated and aged) | 105 | HB(500) | 105 | HB(500) |
Solution temperature | 990 | ºC | 1814 | ºF |
Aging temperature | 470 | ºC | 878 | ºF |
Aging time | 2-4 | hrs. | 2-4 | hrs. |
Liquidus temperature | 1085 | ºC | 1985 | ºF |
Solidus temperature | 1075 | ºC | 1967 | ºF |