Titanium α-β alloy Ti-6Al-2Sn-4Zr-6Mo
Chemical composition: O=0.5% max., Al=6%, Sn=2%, Zr=4%, Mo=6%, Ti balance
Property Value in metric unit Value in US unit
Density 4.65*10³ kg/m³ 290 lb/ft³
Modulus of elasticity 114 GPa 16500 ksi
Thermal expansion (20 ºC) 9.4*10-6 ºCˉ¹ 5.2*10-6 in/(in* ºF)
Specific heat capacity 500 J/(kg*K) 0.12 BTU/(lb*ºF)
Thermal conductivity 7.7 W/(m*K) 52.8 BTU*in/(hr*ft²*ºF)
Electric resistivity 200*10-8 Ohm*m 200*10-6 Ohm*cm
Tensile strength (prec. hard.) 1269 MPa 184000 psi
Yield strength (precip. hard) 1172 MPa 170000 psi
Elongation (precip. hardened) 10 % 10 %
Hardness (precipit. hardened) 41 HRC 41 HRC
Solution temperature 870 ºC 1600 ºF
Aging temperature 590 ºC 1095 ºF
Aging time 4-8 hrs. 4-8 hrs.
Liquidus temperature 1677 ºC 3050 ºF
Solidus temperature 1593 ºC 2900 ºF
Beta Transus temperature 946 ºC 1735 ºF