SubsTech     
SubsTech     
Command disabled: index

to Metals
to Extractive metallurgy

Extractive metallurgy of copper

Dr. Dmitri Kopeliovich

Manufacture of copper and its alloys has a long history of thousands of years.

The basic compounds contained by the copper ores are either copper sulfide or copper oxides.

Copper ores are poor; therefore commercial extraction of copper involves several dressing operations before the smelting stage.

The following technological operations are carried out for copper production from sulfide ores:

  • Crushing and grinding the ore in order to free the gangue from the copper mineral.
  • Concentrating – separation of the copper mineral from the gangue.

This operation is conducted in a flotation chamber where the ground ore mixed with water is treated by air bubbles which move upward and cause flotation of the mineral particles to the top of the chamber.

The copper concentrate formed in this stage contains about 15% of copper.

  • Matte smelting.

At this stage the concentrate is smelted in a reverberatory furnace to produce a mixture of copper and iron, called matte.

The gangue is absorbed by the slag and removed.

  • Blister copper production.

At this stage the matte is converted into molten copper and iron-rich slag by blowing air through the matte.

The resulted copper melt contains about 98% of copper.

  • Casting copper anodes which are used in the followed electrolytic refining stage.
  • Electrolytic refining.

Impure copper anodes are immersed in a sulfuric acid bath. Pure copper foil (starting sheet) serves as the cathode where copper deposits.

Cathodes produced as a result of the electrolytic refining process contain 99.99% of copper.

The pure copper cathodes are used for manufacturing copper and copper alloys products.

to top


Related internal links

extractive_metallurgy_of_copper.txt · Last modified: 2023/12/13 by dmitri_kopeliovich
Promote in SubsTech       Creative Commons License Except where otherwise noted, this work is licensed under a Creative Commons Attribution-Noncommercial-Share Alike 3.0 License