SubsTech     
SubsTech     
Command disabled: index

to Commercially pure nickel alloys
to Properties of nickel alloys

Commercially pure nickel 200

(submitted by the website administration)

Commercially pure nickel 200
Chemical composition: Ni=99% min.
Property Value in metric unit Value in US unit
Density 8.89 *10³ kg/m³ 555 lb/ft³
Modulus of elasticity 207 GPa 30000 ksi
Thermal expansion (20 ºC) 13.3*10-6 ºCˉ¹ 7.4*10-6 in/(in* ºF)
Specific heat capacity 456 J/(kg*K) 0.109 BTU/(lb*ºF)
Thermal conductivity 70.2 W/(m*K) 487 BTU*in/(hr*ft²*ºF)
Electric resistivity 9.5*10-8 Ohm*m 9.5*10-6 Ohm*cm
Tensile strength (annealed) 462 MPa 67000 psi
Yield strength (annealed) 148 MPa 21500 psi
Elongation (annealed) 45 % 45 %
Liquidus temperature 1446 ºC 2635 ºF
Solidus temperature 1436 ºC 2615 ºF