Cast copper special alloy C99400 (Non-Dezincification Alloy)

(submitted by the website administration)

Cast copper alloy C99400 (Non-Dezincification Alloy)
Chemical composition: Ni=2.3%, Fe=2.0%, Al=1.3%, Si=1.3%, Zn=2.8%, Cu=balance
Property Value in metric unit Value in US unit
Density 8.3 *10³ kg/m³ 518 lb/ft³
Modulus of elasticity 133 GPa 19300 ksi
Electric resistivity 14.3*10-8 Ohm*m 14.3*10-6 Ohm*cm
Tensile strength (sand cast) 1000 MPa 145000 psi
Yield strength (sand cast) 606 MPa 88000 psi
Elongation (sand cast) 25 % 25 %
Fatigue strength (sand cast) 331 MPa 48000 psi
Hardness (sand cast) 295 HB(3000) 295 HB(3000)