Cast copper alloy C96970 (Spinodal Bronze ToughMet2 CX)

(submitted by the website administration)

Spinodal Bronze ToughMet2 CX
Chemical composition: Ni=9.0%, Sn=6.0%, Cu=balance
Property Value in metric unit Value in US unit
Density 8.91*10³ kg/m³ 556 lb/ft³
Modulus of elasticity 117 GPa 17000 ksi
Thermal expansion (20 ºC) 16.7*10-6 ºCˉ¹ 9.3*10-6 in/(in* ºF)
Specific heat capacity 381 J/(kg*K) 0.091 BTU/(lb*ºF)
Thermal conductivity 64.9 W/(m*K) 450 BTU*in/(hr*ft²*ºF)
Thermal diffusivity 1.68*10-5 W/(m*K) 0.026 in²/s
Tensile strength (cast and spinodally hardened) 743 MPa 108000 psi
Yield strength (cast and spinodally hardened) 655 MPa 95000 psi
Elongation (cast and spinodally hardened) 7.5 % 7.5 %
Hardness (cast and spinodally hardened) 28 RC 28 RC