Chemical composition: Mg=4.0%, Al balance, sand casting
Property Value in metric unit Value in US unit
Density 2.65 *10³ kg/m³ 165 lb/ft³
Modulus of elasticity 71 GPa 10300 ksi
Thermal expansion (20 ºC) 24.1*10-6 ºCˉ¹ 13.4*10-6 in/(in* ºF)
Specific heat capacity 963 J/(kg*K) 0.230 BTU/(lb*ºF)
Thermal conductivity 138 W/(m*K) 957 BTU*in/(hr*ft²*ºF)
Electric resistivity 4.9*10-8 Ohm*m 4.9*10-6 Ohm*cm
Heat of fusion 3.89*105 J/kg 167 BTU/lb
Liquidus temperature 641 ºC 1185 ºF
Solidus temperature 599 ºC 1110 ºF
Tensile strength (F) 170 MPa 24660 psi
Yield strength (F) 80 MPa 11600 psi
Elongation (F) 5 % 5 %
Shear strength (F) 140 MPa 20300 psi
Fatigue strength (F) 50 MPa 7250 psi
Hardness (F), range 35-65 HB 35-65 HB

Related internal links

Related external links

cast_aluminum_alloy_514.0.txt · Last modified: 2012/06/02 by dmitri_kopeliovich
Promote in SubsTech       Creative Commons License Except where otherwise noted, this work is licensed under a Creative Commons Attribution-Noncommercial-Share Alike 3.0 License