Alloy steels are iron-carbon alloys, to which alloying elements are added with a purpose to improve the steels properties as compared to the Carbon steels.
Due to effect of alloying elements, properties of alloy steels exceed those of plane carbon steels.
AISI/SAE classification divide alloy steels onto groups according to the major alloying elements:
According to the four-digit classification SAE/AISI system:
First digit indicates the class of the alloy steel:
2- Nickel steels;
3- Nickel-chromium steels;
4- Molybdenum steels;
5- Chromium steels;
6- Chromium-vanadium steels;
7- Tungsten-chromium steels;
9- Silicon-manganese steels.
Second digit indicates concentration of the major element in percents (1 means 1%).
Last two digits indicate carbon concentration in 0,01%.
Example: SAE 5130 means alloy chromium steel, containing 1% of chromium and 0.30% of carbon.
| SAE/AISI grade | C, % | Mn,% | P,% max | S,% max | Ni,% | Cr % | Mo% | V% |
|---|---|---|---|---|---|---|---|---|
| 2340 | 0.38-0.43 | 0.70-0.90 | 0.035 | 0.04 | 3.25-3.75 | - | - | - |
| 3115 | 0.13-0.18 | 0.40-0.60 | 0.035 | 0.04 | 1.1-1.4 | 0.55-0.75 | - | - |
| 4027 | 0.25-0.30 | 0.70-0.90 | 0.035 | 0.04 | - | - | 0.20-0.30 | - |
| 4130 | 0.27-0.33 | 0.35-0.60 | 0.035 | 0.04 | - | 0.80-1.15 | 0.15-0.25 | - |
| 4340 | 0.38-0.43 | 0.60-0.80 | 0.035 | 0.04 | 1.65-2.00 | 0.7-0.9 | 0.20-0.30 | - |
| 5140 | 0.38-0.43 | 0.70-0.90 | 0.035 | 0.04 | - | 0.7-0.9 | - | - |
| 6150 | 0.48-0.53 | 0.70-0.90 | 0.035 | 0.04 | - | 0.8-1.1 | - | 0.15 min |
| 8620 | 0.18-0.23 | 0.60-0.90 | 0.035 | 0.04 | 0.40-0.70 | 0.40-0.60 | 0.15-0.25 | - |
| 9255 | 0.51-0.59 | 0.75-1.00 | 0.035 | 0.04 | - | - | - | - |