Wrought magnesium alloy M1A | ||||
Chemical composition: Mn = 1.2% min, Mg balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 1.77 *10³ | kg/m³ | 110 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 45 | GPa | 6530 | ksi |
Thermal expansion (20 ºC) | 26.0*10-6 | ºCˉ¹ | 14.4*10-6 | in/(in* ºF) |
Specific heat capacity | 1000 | J/(kg*K) | 0.239 | BTU/(lb*ºF) |
Thermal conductivity | 139 | W/(m*K) | 964 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 5.0*10-8 | Ohm*m | 5.0*10-6 | Ohm*cm |
Tensile strength (annealed) | 230 | MPa | 33400 | psi |
Yield strength (annealed) | 125 | MPa | 18100 | psi |
Elongation (annealed) | 17 | % | 17 | % |
Shear strength (annealed) | 115 | MPa | 16700 | psi |
Hardness (annealed) | 48 | HB(500) | 48 | HB(500) |
Tensile strength (hard rolled) | 240 | MPa | 34800 | psi |
Yield strength (hard rolled) | 180 | MPa | 26100 | psi |
Elongation (hard rolled) | 7 | % | 7 | % |
Shear strength (hard rolled) | 115 | MPa | 16700 | psi |
Hardness (hard rolled) | 54 | HB(500) | 54 | HB(500) |
Annealing temperature | 371 | ºC | 700 | ºF |
Liquidus temperature | 649 | ºC | 1200 | ºF |
Solidus temperature | 648 | ºC | 1198 | ºF |