to Spinodal Bronzes
to Properties of copper alloys
(submitted by the website administration)
Spinodal Bronze ToughMet3 TS | ||||
Chemical composition: Ni=15.0%, Sn=8.0%, Cu=balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.94*10³ | kg/m³ | 558 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 128 | GPa | 18500 | ksi |
Thermal expansion (20 ºC) | 16.4*10-6 | ºCˉ¹ | 9.1*10-6 | in/(in* ºF) |
Specific heat capacity | 377 | J/(kg*K) | 0.09 | BTU/(lb*ºF) |
Thermal conductivity | 38.1 | W/(m*K) | 264 | BTU*in/(hr*ft²*ºF) |
Thermal diffusivity | 0.9*10-5 | W/(m*K) | 0.014 | in²/s |
Tensile strength (wrought, cold worked and spinodally hardened) | 985 | MPa | 143000 | psi |
Yield strength (wrought, cold worked and spinodally hardened) | 900 | MPa | 130000 | psi |
Elongation (wrought, cold worked and spinodally hardened) | 9 | % | 9 | % |
Hardness (wrought, cold worked and spinodally hardened) | 29.5 | RC | 29.5 | RC |