Weak Base Anion Exchange Resin | ||||
Uniform Particle Size, High Capacity, Weak Base Anion Exchange Resin | ||||
Property | Value in metric unit | Value in US unit | ||
Matrix | Styrene-DVB, macroporous | |||
---|---|---|---|---|
Functional group | Tertiary amine | |||
Exchange capacity | 1.3 | eq/l | 28.4 | kgr of CaCO3/ft³ |
Water content | 55% | |||
Total swelling (Cl- → OH-) | 20% | |||
Mean particle size | 0.53 | mm | 20.9 | μinch |
Particle density | 1.04 | kg/l | 68.1 | lb/ft³ |
Shipping weight | 0.64 | kg/l | 40 | lb/ft³ |
Maximum work temperature | 100 | °C | 212 | °F |
PH range | 0-7 | |||
Min. bed depth | 800 | mm | 2.6 | ft |
Service flow rate | 5-60 | m/h | 2-24 | gpm/ft2 |
Co-current regeneration rinse | 1-10 | m/h | 0.4-4 | gpm/ft2 |
Counter-current regeneration rinse | 5-20 | m/h | 2-8 | gpm/ft2 |
Total rinse requirement | 2-4 bed volumes | |||
Regenerant | NaOH (2-5%) |