Titanium α-β alloy Ti-4Al-4Mo-2Sn | ||||
Chemical composition: O=0.18%, Al=4%, Mo=4%, Sn=2%, Si=0.5%, Ti balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 4.60*10³ | kg/m³ | 287 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 114 | GPa | 16500 | ksi |
Thermal expansion (20 ºC) | 8.8*10-6 | ºCˉ¹ | 4.9*10-6 | in/(in* ºF) |
Thermal conductivity | 7.6 | W/(m*K) | 52.7 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 160*10-8 | Ohm*m | 160*10-6 | Ohm*cm |
Tensile strength | 1138 | MPa | 165000 | psi |
Yield strength | 1035 | MPa | 150000 | psi |
Elongation | 12 | % | 12 | % |
Hardness | 38 | HRC | 38 | HRC |
Solution temperature | 900 | ºC | 1650 | ºF |
Aging temperature | 500 | ºC | 930 | ºF |
Aging time | 4-8 | hrs. | 4-8 | hrs. |
Beta Transus temperature | 975 | ºC | 1787 | ºF |