to Composites
to Polymer Matrix Composites
Dr. Dmitri Kopeliovich
Open Molding (Contact Molding) is the simplest method of fabrication of Polymer Matrix Composites.
Open Molding is usually used for manufacturing large individual parts (swimming pools, boat bodies).
Open Molding method is mostly used for fabrication Glass fiber reinforcing Polymers (Fiberglasses) with polyester (sometimes epoxy or vinylester) matrix.
The methods of open mold fabrication:
The most popular type of Open Molding is Hand Lay-up process. The Hand Lay-up is a manual, slow, labor consuming method, which involves the following operations:
The disadvantages of the Hand Lay-up method are: low concentration of reinforcing phase (up to 30%) and low densification of the composites (entrapped air bubbles).
to top
In Spray-up process liquid resin matrix and chopped reinforcing fibers are sprayed by two separate sprays onto the mold surface.
The fibers are chopped into fibers of 1-2” (25-50 mm) length and then sprayed by an air jet simultaneously with a resin spray at a predetermined ratio between the reinforcing and matrix phase.
The Spray-up method permits rapid formation of uniform composite coating, however the mechanical properties of the material are moderate since the method is unable to use continuous reinforcing fibers.
to top
In this method layers of prepreg (reinforcing phase impregnated by liquid resin) tape are applied on the mold surface by a tape application robot.
to top
Filament Winding method involves a continuous filament of reinforcing material wound onto a rotating mandrel in layers at different layers. If a liquid thermosetting resin is applied on the filament prior to winding the, process is called Wet Filament Winding. If the resin is sprayed onto the mandrel with wound filament, the process is called Dry Filament Winding.
Besides conventional curing of molded parts at room temperature, Autoclave Curing may be used.
to top
Autoclave Curing is a method in which a part, molded by one of the open molding methods, is cured by a subsequent application of vacuum, heat and inert gas pressure.
The molded part is first placed into a plastic bag, from which air is exhausted by a vacuum pump. This operation removes air inclusions and volatile products from the molded part.
Then heat and inert gas pressure are applied in the autoclave causing curing and densification of the material.
Autoclave Curing enables fabrication of consistent homogeneous materials. The method is relatively expensive and is used for manufacturing high quality aerospace products.
to top