Low alloyed titanium, Grade 7 (Ti-0.15Pd) | ||||
Chemical composition: O=0.25% max., Fe=0.3% max., Pd=0.15%, Ti balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 4.51 *10³ | kg/m³ | 282 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 103 | GPa | 15000 | ksi |
Thermal expansion (20 ºC) | 8.6*10-6 | ºCˉ¹ | 4.8*10-6 | in/(in* ºF) |
Specific heat capacity | 520 | J/(kg*K) | 0.124 | BTU/(lb*ºF) |
Thermal conductivity | 20.8 | W/(m*K) | 144 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 56*10-8 | Ohm*m | 56*10-6 | Ohm*cm |
Tensile strength | 434 | MPa | 63000 | psi |
Yield strength | 345 | MPa | 50000 | psi |
Elongation | 20 | % | 20 | % |
Hardness | 82 | HRB | 82 | HRB |
Melting temperature | 1660 | ºC | 3020 | ºF |
Beta Transus temperature | 913 | ºC | 1675 | ºF |