| Commercially pure nickel 270 (high purity nickel) | ||||
| Chemical composition: Ni =99.9% min. | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.89 *10³ | kg/m³ | 555 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 207 | GPa | 30000 | ksi |
| Thermal expansion (20 ºC) | 13.3*10-6 | ºCˉ¹ | 7.4*10-6 | in/(in* ºF) |
| Specific heat capacity | 460 | J/(kg*K) | 0.11 | BTU/(lb*ºF) |
| Thermal conductivity | 86 | W/(m*K) | 597 | BTU*in/(hr*ft²*ºF) |
| Electric resistivity | 7.5*10-8 | Ohm*m | 7.5*10-6 | Ohm*cm |
| Tensile strength (annealed) | 345 | MPa | 50000 | psi |
| Yield strength (annealed) | 110 | MPa | 16000 | psi |
| Elongation (annealed) | 50 | % | 50 | % |
| Liquidus temperature | 1454 | ºC | 2650 | ºF |
| Solidus temperature | 1454 | ºC | 2650 | ºF |