Spinodal Bronze ToughMet2 CX | ||||
Chemical composition: Ni=9.0%, Sn=6.0%, Cu=balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.91*10³ | kg/m³ | 556 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 117 | GPa | 17000 | ksi |
Thermal expansion (20 ºC) | 16.7*10-6 | ºCˉ¹ | 9.3*10-6 | in/(in* ºF) |
Specific heat capacity | 381 | J/(kg*K) | 0.091 | BTU/(lb*ºF) |
Thermal conductivity | 64.9 | W/(m*K) | 450 | BTU*in/(hr*ft²*ºF) |
Thermal diffusivity | 1.68*10-5 | W/(m*K) | 0.026 | in²/s |
Tensile strength (cast and spinodally hardened) | 743 | MPa | 108000 | psi |
Yield strength (cast and spinodally hardened) | 655 | MPa | 95000 | psi |
Elongation (cast and spinodally hardened) | 7.5 | % | 7.5 | % |
Hardness (cast and spinodally hardened) | 28 | RC | 28 | RC |