| Cast aluminum alloy 222.0 | ||||
| Chemical composition: Cu=10.0%, Mg=0.20%, Al balance, sand casting | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 2.95 *10³ | kg/m³ | 184 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 71 | GPa | 10300 | ksi |
| Thermal expansion (20 ºC) | 22.1*10-6 | ºCˉ¹ | 12.3*10-6 | in/(in* ºF) |
| Specific heat capacity | 963 | J/(kg*K) | 0.230 | BTU/(lb*ºF) |
| Thermal conductivity | 130 | W/(m*K) | 902 | BTU*in/(hr*ft²*ºF) |
| Electric resistivity | 5.2*10-8 | Ohm*m | 5.2*10-6 | Ohm*cm |
| Heat of fusion | 3.89*105 | J/kg | 167 | BTU/lb |
| Liquidus temperature | 624 | ºC | 1160 | ºF |
| Solidus temperature | 518 | ºC | 964 | ºF |
| Tensile strength (anneal.),min | 159 | MPa | 23000 | psi |
| Yield strength (annealed),min | 71 | MPa | 10300 | psi |
| Shear strength (annealed) | 99 | MPa | 14400 | psi |
| Hardness (annealed) , range | 65-95 | HB | 65-95 | HB |
| Tensile strength (T61), min | 207 | MPa | 30000 | psi |
| Shear strength (T61) | 127 | MPa | 18400 | psi |
| Hardness (T61) , range | 100-130 | HB | 100-130 | HB |
| Solution temperature | 510 | ºC | 950 | ºF |
| Aging temperature | 154 | ºC | 310 | ºF |
| Aging time | 11 | hrs. | 11 | hrs. |
http://www.tntech.edu/me/courses/Zhang/ME30103110/Chap11pt4.ppt
http://www.ccm.udel.edu/Personnel/homepage/class_web/Lecture%20Notes/2004/AskelandPhuleNotes-
CH13Printable.ppt
http://www.aluminum.org/
http://www.aluminium.org/
http://www.cmse.ed.ac.uk/MSE3/Topics/MSE3-nonferrous.pdf
http://www.ndt-ed.org/GeneralResources/MaterialProperties/ET/et_matlprop_index.htm