| SAE 1006 | ||||
| Chemical composition: C=0.08% max, Mn=0.35% max, P=0.04% max, S=0.05% max | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 200 | GPa | 29000 | ksi |
| Thermal expansion (20 ºC) | 12.6*10-6 | ºCˉ¹ | 7.00*10-6 | in/(in* ºF) |
| Specific heat capacity | 481 | J/(kg*K) | 0.115 | BTU/(lb*ºF) |
| Thermal conductivity | 64.9 | W/(m*K) | 450 | BTU*in/(hr*ft²*ºF) |
| Electric resistivity | 1.40*10-7 | Ohm*m | 1.40*10-5 | Ohm*cm |
| Tensile strength (hot rolled) | 295 | MPa | 42800 | psi |
| Yield strength (hot rolled) | 165 | MPa | 23900 | psi |
| Elongation (hot rolled) | 30 | % | 30 | % |
| Hardness (hot rolled) | 49 | RB | 49 | RB |
| Tensile strength (cold drawn) | 330 | MPa | 47900 | psi |
| Yield strength (cold drawn) | 285 | MPa | 41300 | psi |
| Elongation (cold drawn) | 20 | % | 20 | % |
| Hardness (cold drawn) | 55 | RB | 55 | RB |