to Alloy steels
to Properties of steels and cast irons
(submitted by the website administration)
| SAE 4027 | ||||
| Chemical composition: C=0.40%, Mn=0.8%, Mo=0.25% | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 205 | GPa | 29700 | ksi |
| Thermal expansion (20 ºC) | 12.0*10-6 | ºCˉ¹ | 6.60*10-6 | in/(in* ºF) |
| Specific heat capacity | 477 | J/(kg*K) | 0.114 | BTU/(lb*ºF) |
| Thermal conductivity | 44.6 | W/(m*K) | 309 | BTU*in/(hr*ft²*ºF) |
| Electric resistivity | 2.45*10-7 | Ohm*m | 2.45*10-5 | Ohm*cm |
| Tensile strength (annealed) | 515 | MPa | 74700 | psi |
| Yield strength (annealed) | 325 | MPa | 47100 | psi |
| Elongation (annealed) | 30 | % | 30 | % |
| Hardness (annealed) | 78 | RB | 78 | RB |
| Tensile strength (normalized) | 640 | MPa | 92800 | psi |
| Yield strength (normalized) | 420 | MPa | 60900 | psi |
| Elongation (normalized) | 26 | % | 26 | % |
| Hardness (normalized) | 88 | RB | 88 | RB |