Wrought aluminum-zinc-magnesium alloy 7039 | ||||
Chemical composition: Mn=0.25%, Mg=2.8%, Cr=0.20%, Zn=4.0%, Al balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 2.74 *10³ | kg/m³ | 171 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 70 | GPa | 10100 | ksi |
Thermal expansion (20 ºC) | 23.4*10-6 | ºCˉ¹ | 13.0*10-6 | in/(in* ºF) |
Specific heat capacity | 880 | J/(kg*K) | 0.210 | BTU/(lb*ºF) |
Thermal conductivity | 140 | W/(m*K) | 972 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 4.5*10-8 | Ohm*m | 4.5*10-6 | Ohm*cm |
Tensile strength (annealed) | 230 | MPa | 33400 | psi |
Yield strength (annealed) | 100 | MPa | 14500 | psi |
Elongation (annealed) | 22 | % | 22 | % |
Shear strength (annealed) | 140 | MPa | 20300 | psi |
Hardness (annealed) | 61 | HB | 61 | HB |
Tensile strength (T61) | 400 | MPa | 58000 | psi |
Yield strength (T61) | 330 | MPa | 47900 | psi |
Elongation (T61) | 13 | % | 13 | % |
Shear strength (T61) | 235 | MPa | 34100 | psi |
Fatigue strength (T61) | 160 | MPa | 23200 | psi |
Hardness (T61) | 123 | HB | 123 | HB |
Annealing temperature | 413 | ºC | 775 | ºF |
Solution temperature | 499 | ºC | 930 | ºF |