Chemical composition: Zn=4.5%, Zr = 0.7% min, Mg balance
Property Value in metric unit Value in US unit
Density 1.83 *10³ kg/m³ 114 lb/ft³
Modulus of elasticity 45 GPa 6530 ksi
Thermal expansion (20 ºC) 26.0*10-6 ºCˉ¹ 14.4*10-6 in/(in* ºF)
Specific heat capacity 1020 J/(kg*K) 0.244 BTU/(lb*ºF)
Thermal conductivity 110 W/(m*K) 763 BTU*in/(hr*ft²*ºF)
Electric resistivity 6.2*10-8 Ohm*m 6.2*10-6 Ohm*cm
Tensile strength (T5) 276 MPa 40000 psi
Yield strength (T5) 165 MPa 24000 psi
Elongation (T5) 3 % 3 %
Shear strength (T5) 137 MPa 22000 psi
Hardness (T5) 50 HB(500) 65 HB(500)
Aging temperature 177 ºC 350 ºF
Aging time 12 hrs. 12 hrs.
Liquidus temperature 585 ºC 1085 ºF
Solidus temperature 549 ºC 1020 ºF