Cast magnesium alloy EZ33A
Chemical composition: Nd=3.2%, Zn=2.6%, Zr = 0.7% min, Mg balance
Property Value in metric unit Value in US unit
Density 1.80 *10³ kg/m³ 112 lb/ft³
Modulus of elasticity 45 GPa 6530 ksi
Thermal expansion (20 ºC) 26.4*10-6 ºCˉ¹ 14.7*10-6 in/(in* ºF)
Specific heat capacity 1040 J/(kg*K) 0.249 BTU/(lb*ºF)
Thermal conductivity 99.5 W/(m*K) 691 BTU*in/(hr*ft²*ºF)
Electric resistivity 7.0*10-8 Ohm*m 7.0*10-6 Ohm*cm
Tensile strength (T5) 159 MPa 23000 psi
Yield strength (T5) 110 MPa 16000 psi
Elongation (T5) 3 % 3 %
Shear strength (T5) 137 MPa 19800 psi
Hardness (T5) 50 HB(500) 50 HB(500)
Aging temperature 215 ºC 420 ºF
Aging time 5 hrs. 5 hrs.
Liquidus temperature 643 ºC 1189 ºF
Solidus temperature 543 ºC 1010 ºF