to Cast copper special alloys
to Properties of copper alloys

Cast copper special alloy C99750


Cast copper special alloy C99750
Chemical composition: Mn=20%, Al=1.6%, Zn=20%, Pb=1.5%, Cu=57%
Property Value in metric unit Value in US unit
Density 8.03 *10³ kg/m³ 501 lb/ft³
Modulus of elasticity 117 GPa 17000 ksi
Thermal expansion (20 ºC) 24.3*10-6 ºCˉ¹ 13.5*10-6 in/(in* ºF)
Specific heat capacity 377 J/(kg*K) 0.09 BTU/(lb*ºF)
Electric resistivity 83.8*10-8 Ohm*m 83.8*10-6 Ohm*cm
Tensile strength (sand cast) 448 MPa 65000 psi
Yield strength (sand cast) 221 MPa 32000 psi
Elongation (sand cast) 30 % 30 %
Fatigue strength (sand cast) 128 MPa 19000 psi
Hardness (sand cast) 110 HB(500) 110 HB(500)
Tensile strength (quenched+annealed) 517 MPa 75000 psi
Yield strength (quenched+annealed) 276 MPa 40000 psi
Elongation (quenched+annealed) 20 % 20 %
Hardness (quenched+annealed) 119 HB(500) 119 HB(500)
Liquidus temperature 843 ºC 1550 ºF
Solidus temperature 818 ºC 1505 ºF