Cast copper alloy C95500 (Aluminum Bronze) | ||||
Chemical composition: Al=11.0%, Fe=4.0%, Ni=4.3%, Cu=81.7% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.53 *10³ | kg/m³ | 470 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 110 | GPa | 16000 | ksi |
Thermal expansion (20 ºC) | 16.2*10-6 | ºCˉ¹ | 9.0*10-6 | in/(in* ºF) |
Specific heat capacity | 419 | J/(kg*K) | 0.10 | BTU/(lb*ºF) |
Thermal conductivity | 41.9 | W/(m*K) | 290 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 20.4*10-8 | Ohm*m | 20.4*10-6 | Ohm*cm |
Tensile strength (sand cast) | 689 | MPa | 100000 | psi |
Yield strength (sand cast) | 303 | MPa | 44000 | psi |
Elongation (sand cast) | 12 | % | 12 | % |
Shear strength (sand cast) | 331 | MPa | 48000 | psi |
Fatigue strength (sand cast) | 214 | MPa | 31000 | psi |
Hardness (sand cast) | 195 | HB(3000) | 195 | HB(3000) |
Tensile strength (sand cast and quenched) | 827 | MPa | 120000 | psi |
Yield strength (sand castand quenched) | 469 | MPa | 68000 | psi |
Elongation (sand castand quenched) | 10 | % | 10 | % |
Shear strength (sand castand quenched) | 483 | MPa | 70000 | psi |
Fatigue strength (sand cast and quenched) | 262 | MPa | 38000 | psi |
Hardness (sand castand quenched) | 230 | RB | 230 | RB |
Liquidus temperature | 1054 | ºC | 1930 | ºF |
Solidus temperature | 1038 | ºC | 1900 | ºF |